• ISSN 1001-1455  CN 51-1148/O3
  • EI、Scopus、CA、JST、EBSCO、DOAJ收录
  • 力学类中文核心期刊
  • 中国科技核心期刊、CSCD统计源期刊

超低温冲击下钛合金局部化塑性失稳

陈美多,  黄婷婷,  熊颖,  冯浩然,  王鹏飞,  徐松林

陈美多, 黄婷婷, 熊颖, 冯浩然, 王鹏飞, 徐松林. 超低温冲击下钛合金局部化塑性失稳[J]. 爆炸与冲击. doi: 10.11883/bzycj-2025-0390
引用本文: 陈美多, 黄婷婷, 熊颖, 冯浩然, 王鹏飞, 徐松林. 超低温冲击下钛合金局部化塑性失稳[J]. 爆炸与冲击. doi: 10.11883/bzycj-2025-0390
CHEN Meiduo, HUANG Tingting, XIONG Ying, FENG Haoran, WANG Pengfei, XU Songlin. Localized plastic instability of titanium alloy under mechanical impact at ultra-low temperature[J]. Explosion And Shock Waves. doi: 10.11883/bzycj-2025-0390
Citation: CHEN Meiduo, HUANG Tingting, XIONG Ying, FENG Haoran, WANG Pengfei, XU Songlin. Localized plastic instability of titanium alloy under mechanical impact at ultra-low temperature[J]. Explosion And Shock Waves. doi: 10.11883/bzycj-2025-0390

超低温冲击下钛合金局部化塑性失稳

doi: 10.11883/bzycj-2025-0390
基金项目: 国家自然科学基金(11872361,12372372,W2542019);安徽省自然科学基金(1708085MA05)
详细信息
    作者简介:

    陈美多(1999- ),男,博士研究生,mdchen@mail.ustc.edu.cn

    通讯作者:

    徐松林(1971- ),男,博士,研究员,博士生导师. slxu99@ustc.edu.cn

  • 中图分类号: O382

Localized plastic instability of titanium alloy under mechanical impact at ultra-low temperature

  • 摘要: 基于液氦制冷系统对钛合金试样进行了霍普金森冲击压缩实验,研究了低至液氦温区(30 K)的钛合金动态性能及失稳特性。钛合金试样采用圆环形结构,有利于剪切带产生。实验结果表明:低温增强了钛合金的动态强度;材料整体上表现出脆性变形特征,且低温使得钛合金中剪切带更容易产生;剪切带宽度随着温度的降低逐渐变窄。结合基于广义变分原理建立的局部动态失稳控制方程和考虑局部微结构演化的本构关系,研究了局部化剪切带的三个发展阶段。结果表明:低温改变了材料的塑性刚度,促使剪切带在更低应变下产生;剪切带在应力应变曲线峰值点之前形成。
  • 图  1  超低温动态实验装置

    Figure  1.  Ultra low temperature dynamic experimental device

    图  2  超低温真空实验腔体

    Figure  2.  Ultra-low temperature vacuum test chamber

    图  3  钛合金圆环试样

    Figure  3.  The lateral inertia of the sample

    图  4  钛合金圆环在30 K环境下的波形图和应力平衡

    Figure  4.  Waveform diagram and stress balance of titanium alloy rings in a 30 K environment

    图  5  三种温度下钛合金试样应力应变曲线和宏观失效特性

    Figure  5.  Stress strain curves and macroscopic failure characteristics of titanium alloy specimens at three different

    图  6  三种温度下钛合金试样微观失效特性

    Figure  6.  Microscopic failure characteristics of titanium alloy samples at three temperatures

    图  7  不同温度下应力应变曲线特性

    Figure  7.  Engineering tress-strain curves under different temperature

    图  8  钛合金圆环剪切带形貌

    Figure  8.  Shear band morphology of titanium alloy rings

    图  9  剪切带宽度随温度和应变率变化

    Figure  9.  The width of the shear band varies with temperature and strain rate.

    图  10  剪切带角度随温度和应变率的变化

    Figure  10.  Angle of the shear band varies with temperature and strain rate

    图  11  剪切局部化失稳示意图

    Figure  11.  Schematic diagram of localized shear instability

    图  12  2200 s−1下钛合金剪切带演化

    Figure  12.  ASB Formation in titanium alloy at strain rate 2200 s−1

    图  13  2200 s−1下钛合金塑性模量图

    Figure  13.  Plastic modulus in titanium alloy at strain rate 2200 s−1

    图  14  2000 s−1应变率,30 K温度下钛合金剪切带演化图

    Figure  14.  ASB Formation in titanium alloy at the strain rate 2200 s−1 and the temperature of 30 K

    图  15  应变率为2200 s-1时的剪切带演化

    Figure  15.  Shear band evolution at 2200 s-1

    图  16  临界点(B)与应力峰值点(C)的应变比

    Figure  16.  Strain ratio between the critical point (B) and the peak stress point (C)

    表  1  Ti-6AL-4V在常温准静态加载下的基本物理力学性能

    Table  1.   Basic physical and mechanical properties of Ti-6AL-4V under quasi-static loading at room temperature

    材料密度/(kg·m−3)模量/GPa泊松比屈服强度/MPa拉伸强度/MPa热导率/(W·m−1·K−1)比热容/(J·kg−1·K−1)
    Ti-6AL-4V45001090.349109856.8611
    下载: 导出CSV

    表  2  钛合金低温动态实验结果汇总

    Table  2.   Summary of dynamic experimental results of titanium alloy rings

    温度/K 冲击速度/(m·s−1) 应变率/s−1 屈服应力/MPa 峰值应力/MPa 峰值应变 剪切带角度/(°) 剪切带宽度/μm
    29812.315001237.971396.050.0680No ASB
    16.722001224.151534.280.123847.4~60.99.42
    22.830001248.501614.210.128756.9~77.713.42
    26.860001274.751635.700.1082Shear failure
    35.270001314.781682.120.1021Shear failure
    7714.412001186.881413.880.092No ASB
    17.722001263.591563.310.100844.3~52.86.59
    23.428001280.331582.880.102054.8~58.57.24
    28.832001169.451694.300.155749.5~59.37.04
    32.544001288.921700.670.124450.0~59.37.64
    34.346001321.271746.510.122852.7~61.18.28
    3016.315001446.801761.530.113940.2~66.82.7
    20.820001384.501791.550.173146.4~57.20.5~2.0/4.2~8.5
    23.725001596.981806.660.107455.1~64.93.5-4.8
    36.532001494.931977.860.1045Shear failure
    下载: 导出CSV
  • [1] ZHU Y M, ZHANG K, MENG Z C, et al. Ultrastrong nanotwinned titanium alloys through additive manufacturing [J]. Nature Materials, 2022, 21(11): 1258–1262. DOI: 10.1038/s41563-022-01359-2.
    [2] LI Q, HUANG S, ZHAO Y K, et al. Simultaneous enhancements of strength, ductility, and toughness in a TiB reinforced titanium matrix composite [J]. Acta Materialia, 2023, 254: 118995. DOI: 10.1016/j.actamat.2023.118995.
    [3] LI Y X, WANG L, AN R, et al. Deformation behavior of Ti-6Al-3Nb-2Zr-1Mo titanium alloy at low temperatures and high strain rates [J]. Rare Metal Materials and Engineering, 2022, 51(12): 4369–4375. DOI: 10.12442/j.issn.1002-185X.20220181.
    [4] SU W L, WANG M S, GUO F J, et al. Heterostructure enables anomalous improvement of cryogenic mechanical properties in titanium [J]. Acta Materialia, 2024, 273: 119982. DOI: 10.1016/j.actamat.2024.119982.
    [5] 陈美多, 张祥林, 袁良柱, 等. 岩石界面的动态剪切扩散行为 [J]. 爆炸与冲击, 2024, 44(8): 081422. DOI: 10.11883/bzycj-2023-0469.

    CHEN M D, ZHANG X L, YUAN L Z, et al. Dynamic shear diffusion behavior at rock interfaces [J]. Explosion and Shock Waves, 2024, 44(8): 081422. DOI: 10.11883/bzycj-2023-0469.
    [6] CHAUSOV M, MARUSCHAK P, PYLYPENKO A, et al. Changes in the mechanical properties and structural condition of stainless steel AISI 301 caused by the combined effect of impact-oscillatory loading and cryogenic cooling. Effects caused by holding specimens in liquid nitrogen for 1 h [J]. Vacuum, 2025, 240: 114541. DOI: 10.1016/j.vacuum.2025.114541.
    [7] CUI Z Y, LIU F Y, XUE J L, et al. Quasi-static and dynamic deformation behavior of low alloy steel at room and low temperatures [J]. Materials Science and Engineering: A, 2025, 943: 148776. DOI: 10.1016/j.msea.2025.148776.
    [8] WANG K Y, CHENG Z J, LIU C Y, et al. Deformation behavior and strengthening mechanisms of high-entropy alloys under high strain rate across wide temperature ranges [J]. International Journal of Plasticity, 2025, 189: 104321. DOI: 10.1016/j.ijplas.2025.104321.
    [9] LIU D, YU Q, KABRA S, et al. Exceptional fracture toughness of CrCoNi-based medium-and high-entropy alloys at 20 kelvin [J]. Science, 2022, 378(6623): 978–983. DOI: 10.1126/science.abp8070.
    [10] SUN H L, HUO M W, HU X W, et al. Signatures of superconductivity near 80 K in a nickelate under high pressure [J]. Nature, 2023, 621(7979): 493–498. DOI: 10.1038/s41586-023-06408-7.
    [11] SUN Q Y, GU H C. Tensile and low-cycle fatigue behavior of commercially pure titanium and Ti–5Al–2.5Sn alloy at 293 and 77 K [J]. Materials Science and Engineering: A, 2001, 316(1/2): 80–86. DOI: 10.1016/S0921-5093(01)01249-7.
    [12] ZANG M C, NIU H Z, YU J S, et al. Cryogenic tensile properties and deformation behavior of a fine-grained near alpha titanium alloy with an equiaxed microstructure [J]. Materials Science and Engineering: A, 2022, 840: 142952. DOI: 10.1016/j.msea.2022.142952.
    [13] SEMENOVA I P, MODINA J, POLYAKOV A V, et al. Charpy absorbed energy of ultrafine-grained Ti-6Al-4V alloy at cryogenic and elevated temperatures [J]. Materials Science and Engineering: A, 2019, 743: 581–589. DOI: 10.1016/j.msea.2018.10.076.
    [14] WANG Q G, LIU X Y, REN Y J, et al. Microstructural evolution and cryogenic and ambient temperature deformation behavior of the near-α titanium alloy TA15 fabricated by laser powder bed fusion [J]. Journal of Alloys and Compounds, 2024, 1001: 175075. DOI: 10.1016/j.jallcom.2024.175075.
    [15] 包合胜, 王礼立, 卢维娴. 钛合金在低温下的高速变形特性和绝热剪切 [J]. 爆炸与冲击, 1989, 9(2): 109–119. DOI: 10.11883/1001-1455(1989)02-0109-11.

    BAO H S, WANG L L, LU W X. The high velocity deformation and adiabatic shearing of a titanium alloy at low temperature [J]. Explosion and Shock Waves, 1989, 9(2): 109–119. DOI: 10.11883/1001-1455(1989)02-0109-11.
    [16] CAPPOLA J, STINVILLE J C, CHARPAGNE M A, et al. On the localization of plastic strain in microtextured regions of Ti-6Al-4V [J]. Acta Materialia, 2021, 204: 116492. DOI: 10.1016/j.actamat.2020.116492.
    [17] LI Z Z, ZHAO S T, WANG B F, et al. The effects of ultra-fine-grained structure and cryogenic temperature on adiabatic shear localization in titanium [J]. Acta Materialia, 2019, 181: 408–422. DOI: 10.1016/j.actamat.2019.09.011.
    [18] LIU R Y, YU X Y, LI W S, et al. Effects of cryogenic temperature on adiabatic shear localization in equiatomic NiCrFe medium-entropy alloy [J]. Journal of Materials Engineering and Performance, 2025, 34(8): 6867–6878. DOI: 10.1007/s11665-024-09672-4.
    [19] JIANG K, LI J G, KAN X K, et al. Adiabatic shear localization induced by dynamic recrystallization in an FCC high entropy alloy [J]. International Journal of Plasticity, 2023, 162: 103550. DOI: 10.1016/j.ijplas.2023.103550.
    [20] ZHAO F, WANG L, FAN D, et al. Macrodeformation twins in single-crystal aluminum [J]. Physical Review Letters, 2016, 116(7): 075501. DOI: 10.1103/PhysRevLett.116.075501.
    [21] LIU M, WANG P F, LU G X, et al. Deformation-activated recrystallization twin: new twinning path in pure aluminum enabled by cryogenic and rapid compression [J]. iScience, 2022, 25(5): 104248. DOI: 10.1016/j.isci.2022.104248.
    [22] 张磊, 王文帅, 苗春贺, 等. 花岗岩粗糙表面动摩擦形态演化 [J]. 高压物理学报, 2021, 35(3): 031201. DOI: 10.11858/gywlxb.20200640.

    ZHANG L, WANG W S, MIAO C H, et al. Rough surface morphology of granite subjected to dynamic friction [J]. Chinese Journal of High Pressure Physics, 2021, 35(3): 031201. DOI: 10.11858/gywlxb.20200640.
    [23] CHEN M D, XU S L, YUAN L Z, et al. Influence of stress state on dynamic behaviors of concrete under true triaxial confinements [J]. International Journal of Mechanical Sciences, 2023, 253: 108399. DOI: 10.1016/j.ijmecsci.2023.108399.
    [24] CHEN M D, ZHANG X L, XU S L, et al. Dynamic failure of aramid paper honeycomb under intermediate strain rate loading [J]. Thin-Walled Structures, 2025, 215: 113362. DOI: 10.1016/j.tws.2025.113362.
    [25] 简世豪, 苗春贺, 张磊, 等. 双石英玻璃珠的低速冲击破碎行为 [J]. 高压物理学报, 2021, 35(2): 024202. DOI: 10.11858/gywlxb.20200629.

    JIAN S H, MIAO C H, ZHANG L, et al. Fragmentation of double quartz glass spheres subjected to lower-velocity impact [J]. Chinese Journal of High Pressure Physics, 2021, 35(2): 024202. DOI: 10.11858/gywlxb.20200629.
    [26] FORRESTAL M J, WRIGHT T W, CHEN W. The effect of radial inertia on brittle samples during the split Hopkinson pressure bar test [J]. International Journal of Impact Engineering, 2007, 34(3): 405–411. DOI: 10.1016/j.ijimpeng.2005.12.001.
    [27] LI Q M, LU Y B, MENG H. Further investigation on the dynamic compressive strength enhancement of concrete-like materials based on split Hopkinson pressure bar tests. Part II: Numerical simulations [J]. International Journal of Impact Engineering, 2009, 36(12): 1335–1345. DOI: 10.1016/j.ijimpeng.2009.04.010.
    [28] 施春英, 徐松林, 单俊芳, 等. 纵向冲击压缩下LY12铝合金圆环的塑性失稳 [J]. 爆炸与冲击, 2017, 37(3): 471–478. DOI: 10.11883/1001-1455(2017)03-0471-08.

    SHI C Y, XU S L, SHAN J F, et al. Plastic instability of LY12 aluminum alloy ring under longitudinal impact compression [J]. Explosion and Shock Waves, 2017, 37(3): 471–478. DOI: 10.11883/1001-1455(2017)03-0471-08.
    [29] WANG P F, JIANG H B, XU S L, et al. Dynamic plastic instability of ring-shaped aluminum alloy with different interface behaviors [J]. International Journal of Impact Engineering, 2021, 155: 103898. DOI: 10.1016/j.ijimpeng.2021.103898.
    [30] LI G C, ZHU C. Formation of shear bands in plane sheet [J]. International Journal of Plasticity, 1995, 11(5): 605–622. DOI: 10.1016/S0749-6419(95)00025-9.
    [31] GUO Y Z, RUAN Q C, ZHU S X, et al. Temperature rise associated with adiabatic shear band: causality clarified [J]. Physical Review Letters, 2019, 122(1): 015503. DOI: 10.1103/PhysRevLett.122.015503.
    [32] GUO Y Z, RUAN Q C, ZHU S X, et al. Dynamic failure of titanium: temperature rise and adiabatic shear band formation [J]. Journal of the Mechanics and Physics of Solids, 2020, 135: 103811. DOI: 10.1016/j.jmps.2019.103811.
    [33] RITTEL D, WANG Z G, MERZER M. Adiabatic shear failure and dynamic stored energy of cold work [J]. Physical Review Letters, 2006, 96(7): 075502. DOI: 10.1103/PhysRevLett.96.075502.
    [34] HILL R, HUTCHINSON J W. Bifurcation phenomena in the plane tension test [J]. Journal of the Mechanics and Physics of Solids, 1975, 23(4/5): 239–264. DOI: 10.1016/0022-5096(75)90027-7.
    [35] SINGH G, BAJARGAN G, DATTA R, et al. Deformation and strength of Ti–6Al–4V alloyed with B at cryogenic temperatures [J]. Materials Science and Engineering: A, 2014, 611: 45–57. DOI: 10.1016/j.msea.2014.05.075.
    [36] NAYAN N, SINGH G, ANTONY PRABHU T, et al. Cryogenic mechanical properties of warm multi-pass caliber-rolled fine-grained titanium alloys: Ti-6Al-4V (normal and ELI grades) and VT14 [J]. Metallurgical and Materials Transactions A, 2018, 49(1): 128–146. DOI: 10.1007/s11661-017-4417-y.
  • 加载中
图(16) / 表(2)
计量
  • 文章访问数:  624
  • HTML全文浏览量:  93
  • PDF下载量:  81
  • 被引次数: 0
出版历程
  • 收稿日期:  2025-12-02
  • 修回日期:  2026-01-26
  • 网络出版日期:  2026-01-30

目录

    /

    返回文章
    返回